Which Magnetic Tests Should a Certificate Report?
A single loss figure gets quoted on the phone and settles nothing. Magnetic test items fill seven lines on a certificate, and each line answers a different question. Jiangsu Zhongtong Weiye Special Steel Co., Ltd. walks that sheet below, using a grain oriented sheet as the example.
The Short Answer
Loss, flux density, stacking factor, resistance, adhesion, dimensions, and appearance cover a shipment, as the test method list shows. Seven lines then describe a sheet, while one line leaves gaps. Hence a buyer should ask for all seven, and read each basis before trusting a number. The basis note covers the naming trap.
Line One — Specific Total Loss
Loss is reported in watts per kilogram, at a stated flux density and frequency. A 1.5 T basis and a 1.7 T basis therefore give two numbers for one sheet. A grade of 4.70 W/kg at 1.5 T cannot be compared with 1.20 W/kg at 1.7 T. The fields differ, so the numbers cannot meet. Hence the basis belongs beside the number, each time. The loss note separates the terms inside it.
Line Two — Flux Density
Flux density is reported in tesla at a stated field strength, although the notation hides a trap. Sheets print B800 for 800 amperes per metre, while some print B8 for that same point. A buyer who reads B8 as 8 amperes per metre gets a meaningless comparison. The two fields differ by 100 times. Hence the field strength belongs beside the number too. An oriented grade therefore runs near 1.85 to 1.95 T at that point.
Line Three — Stacking Factor
Stacking factor is a ratio, so it carries no units. A stack of nominal 270 mm usually builds near 96 percent of that height, because the coating takes up space. A low factor therefore inflates the computed flux density, and that flatters the loss reading. Hence the factor and the build height should travel together, rather than apart. The stacking note covers the arithmetic.
Line Four — Interlamination Resistance
Interlamination resistance is reported in ohm square centimetres, since it describes the coating rather than the steel. A value in the hundreds to thousands indicates a sound film, while a value near zero signals bridging. A value near zero indicates bridging, so it reads as a scrap signal rather than a grade signal. Hence this line catches what loss cannot show, and a cut core coupon settles it in minutes. The method follows IEC 60404-11.
Line Five — Coating Adhesion
Adhesion is judged by a bend or a tape pull, so it produces a pass or a fail. A film that lifts on a bend will fail in a press, because the punch peels it. Hence adhesion protects the next process, and it earns a line of its own. The stamping note covers what a press does to a weak film.
Line Six — Dimensions
Dimensions cover thickness, width, camber, and burr, while each carries a tolerance. Thickness runs within plus or minus 5 percent, so a 0.50 mm sheet spans 0.475 to 0.525. Burr stays under 0.02 mm, because a taller burr bridges the film. Hence dimensions decide whether the magnetic lines can be trusted at all. The burr note covers that limit.
Line Seven — Appearance
Appearance covers colour, stains, scratches, and edge condition, so it needs a written standard. A yellow tint may signal oxidation, whereas a scratch may signal handling damage. Neither shows in a loss number, although both change a verdict. Hence appearance belongs on the sheet, even when it reads as opinion. The colour note covers the tint.
How the Sample Is Cut
An Epstein frame takes strips 25 centimetres long and 30 millimetres wide, so it needs about one kilogram. A 0.50 mm sheet yields roughly 0.255 square metres per kilogram, so a full set runs near 34 strips. A single sheet tester instead uses one 500 mm square, since it suits a quick check. Hence the method decides the sample, and a free sample settles the method before the order.
What Goes Wrong
One buyer compares a 1.5 T figure with a 1.7 T figure, then rejects a sound coil. Another reads B8 as a low field, so a grade gets misjudged. A third accepts a certificate without a stacking factor, so nobody can check the build. Those three errors arrive monthly, as the FAQ page notes.

What We Do Not Do
We do not melt or roll steel. We do not test a customer’s finished core, because that test belongs to the builder. Nor do we print a loss figure without its basis, since the basis carries the meaning.
Those limits keep the answer honest, and they keep a certificate readable.
Specify Your Order
Give the grade, the basis, the coating class, and the tolerance. Those four fields then set the certificate. Add the test method, because a frame result and a single sheet result differ slightly. A CRGO coil arrives with a coil report. A cut core arrives with a stack report. That reply usually takes a day.
Related Reading
Our measurement note covers the flux side. The CT note covers a low flux duty. A hub page answers six basic questions.
Frequently Asked Questions
Seven, and each should carry its basis, since a bare number misleads.
Because 1.5 T and 1.7 T give different numbers for one sheet.
Flux density at 800 amperes per metre, which some sheets print as B8.
A bridged coating, which points to scrap rather than a weak grade.
About one kilogram of 25 centimetre strips, or roughly 34 pieces.
- Email: vera.liang@ztwysteel.com
- Location: Xishan District, Wuxi, Jiangsu, China
- Supply range: CRGO and CRNGO 0.20–0.65 mm, four coating classes
- Slitting: 20–1,250 mm, ±0.05 mm, burr under 0.02 mm
- Documentation: MTC EN 10204 3.1 with grade, thickness and loss basis, 3.2 on request