50W470 Non-Oriented Silicon Steel: Properties That Matter
50W470 is a 0.50 mm thick non-oriented electrical steel with a guaranteed core loss ceiling of 4.70 W/kg at 1.5 T, 50 Hz. It sits in the middle of the 0.50 mm band: better than 50W600 and 50W800, but not as efficient as 50W400 or thinner high-grade material. This page sets out its guaranteed magnetic values, the mechanical limits that decide how it punches and stacks, and where the grade is worth specifying. It is part of the wider non-oriented electrical steel range.
Reading the Grade Code
Under GB/T 2521.1, the code carries three facts:
- 50is the nominal thickness times 100, so 0.50 mm.
- Wmarks non-oriented electrical steel, where properties are roughly uniform in the plane rather than aligned to one rolling direction.
- 470is the maximum specific total loss at 1.5 T and 50 Hz, P1.5/50, times 100, so a ceiling of 4.70 W/kg.
Note that non-oriented grades are measured at 1.5 T, not the 1.7 T used for oriented steel. A 4.70 W/kg figure quoted on this grade cannot be compared with an oriented grade’s 1.17 W/kg number without converting the test point. How CRNGO grade codes read covers the same logic in the American M-series notation, where this band corresponds to roughly M470-50A.
Guaranteed Magnetic Values
The values below come from the GB/T 2521.1 grade table, so they are the limits a supplier must meet rather than typical figures:
| Property | Value for 50W470 |
| Nominal thickness | 0.50 mm |
| Conventional density | 7.70 kg/dm³ |
| P1.5/50, maximum | 4.70 W/kg |
| P1.5/60, maximum | 5.90 W/kg |
| J2500, reference | 1.54 T |
| J5000, minimum | 1.65 T |
| J10000, reference | 1.74 T |
| Loss anisotropy | ±10% |
| Minimum bend count | 10 |
| Minimum stacking factor | 0.97 |
Two entries deserve attention. J5000 at 1.65 T is the guaranteed induction figure, and it is the one to compare against the design’s working flux. The anisotropy tolerance of ±10% means the loss measured across the rolling direction can run up to 10% above the with-rolling figure; a core that mixes transverse and longitudinal paths should be sized on the higher end. The M-series grade comparison puts this band next to its neighbours.

Where the Loss Sits Against Neighbouring Grades
Reading the 0.50 mm band in order:
| Grade | P1.5/50 max | J5000 min | Density |
| 50W400 | 4.00 W/kg | 1.64 T | 7.70 |
| 50W470 | 4.70 W/kg | 1.65 T | 7.70 |
| 50W600 | 6.00 W/kg | 1.67 T | 7.75 |
| 50W800 | 8.00 W/kg | 1.70 T | 7.80 |
The pattern is worth noting: as the loss ceiling drops, the induction minimum drops too, and density falls as silicon content rises. Higher grades are not simply “better on all axes”; they trade induction and saturating behaviour for lower loss. That is why a design working at high flux may prefer 50W600 over 50W470 despite the worse loss figure.
Mechanical Limits and Yield Strength
GB/T 2521.1 sets mechanical properties as an informative annex, not a guaranteed requirement, and it specifies only tensile strength and elongation:
| Property | 50W470 |
| Tensile strength Rm, minimum | 380 MPa |
| Elongation A50mm, minimum | 16% |
Yield strength is not a standard value. It is a mill data-sheet item and has to be requested from the supplier for the specific lot. On commercial 50W470 material it is commonly quoted in the 250 to 350 MPa band, moving with silicon content, rolling route and annealing. For die design, blanking force and springback calculations, ask for the mill’s own Rp0.2 rather than using a generic figure.
The mechanical direction of travel across the grade band is consistent: lower loss means more silicon, which raises yield strength, raises hardness and cuts elongation. Punched motor laminations therefore face a real trade-off. A 50W800 grade punches easily and wears tooling less, while 50W470 needs tighter die maintenance and a blanking setup that does not strain the sheet at the sheared edge.
Punching, Burr and Stacking
Three processing points decide how much of the grade’s magnetic advantage actually reaches the finished core:
- Burr height.A dull die leaves burr that bridges laminations and creates local short circuits between sheets. On 0.50 mm material the burr allowance is tighter than on thicker gauge, and the loss penalty can erase the gain from choosing a lower-loss grade.
- Stress from shearing.Punching introduces plastic strain near the cut edge, which raises local loss. Annealing after punching recovers part of it; the recovery is larger on higher-silicon grades, which is one reason stress-relief annealing is often specified for efficient motors.
- Stacking factor.The guaranteed 0.97 applies to uncoated condition in case of dispute. Coating thickness, burr and surface flatness all pull the achieved factor below the standard figure, and the shortfall shows up directly as lower flux for the same core volume.
Where 50W470 Fits
The grade suits induction motors and generators in the small to medium frame range, home appliance and compressor motors, and general industrial drives where the efficiency class leaves some loss headroom. It is a common choice for 50 Hz machines built to a normal efficiency target, and for cores that need decent induction as well as acceptable loss.
It is the wrong choice in two situations: when the efficiency class is tight enough that the loss ceiling has to come down further, and when the design runs at high flux where 50W600’s higher induction is worth more than 50W470’s lower loss. Thicker against thinner gauge in motor cores covers the gauge decision, and selecting non-oriented steel for motors covers the wider grade selection.
FAQ
Is 50W470 the same as M470-50A? They sit in the same band but are not identical documents. M470-50A is the American notation for 0.50 mm, 4.70 W/kg class material; always match on the certificate values rather than the name.
Can 50W470 be compared with oriented steel on core loss? Only after converting the test point. 50W470 is measured at 1.5 T while oriented CRGO grades are measured at 1.7 T, so the raw numbers are not on the same basis.
Does a lower loss grade always give higher induction? No. In the 0.50 mm band, lower loss generally comes with lower J5000 and lower density, so a high-flux design may do better on a higher-loss grade.
What yield strength should I design tooling for? Ask the mill for the lot’s Rp0.2. GB/T 2521.1 does not guarantee yield strength; only tensile strength and elongation appear in the annex.
Does 50W470 need stress-relief annealing after punching? It depends on the loss target. Annealing after punching recovers part of the shearing strain, and the recovery is larger on higher-silicon grades, so tight-loss designs usually specify it.
Working on a 0.50 mm motor or generator core? Send the frame size, working flux and efficiency class to vera.liang@ztwysteel.com, and we will confirm the grade band, coating and certificate values for the design. The silicon electrical steel sheet range shows the stocked gauges.