What is the difference between Monel 400 and Monel K500?
The gap sits in the process, not only in the chemistry. Monel K500 doubles the yield of 400 yet changes the route. 400 forms and then serves. K500 forms, ages, and only then gets machined. Jiangsu Zhongtong Weiye Special Steel Co., Ltd. stocks K500 bar, and it quotes 400 plate on request.
The Short Answer
400 reaches about 240 MPa yield in the annealed state, while K500 reaches near 690 MPa after ageing. Both keep the nickel-copper corrosion behaviour. Hence a designer picks K500 for load and 400 for cost.
The Chemistry Delta
K500 starts from the same nickel-copper base, then adds aluminium and titanium, roughly 0.5 to 1% of each. Those two elements age into a fine precipitate. 400 carries neither, so it stays soft at any condition. Therefore, one small addition explains the whole strength gap.
The Strength Gap
An annealed 400 part yields near 240 MPa, and its tensile sits near 550 MPa. An aged K500 part yields near 690 MPa, with tensile near 965 MPa. That factor of nearly three allows a thinner shaft at the same torque. Hence a pump maker often switches on strength alone.
The Sequence Difference
400 needs no heat treatment after forming, so a fabricator cuts, bends, and ships. K500 needs a age cycle near 540 °C for several hours after forming, and the part then scales slightly. A finished dimension must therefore allow for that growth. Hence the schedule changes, not only the alloy.
What the Age Does to Size
Ageing grows a K500 part by a small amount, and a long shaft grows more than a short one. A machined-to-size shaft would drift out of tolerance after the cycle. The usual route rough-machines, ages, then finishes, which the cut-to-size note covers at the sheet stage. Therefore, the drawing should carry an intermediate dimension.
The Welding Difference
400 welds with a matching filler and needs no post-weld treatment. K500 welds with a nickel-copper filler. The joint then ages with the part, since the weld zone stays soft otherwise. A welded K500 assembly therefore enters the furnace after fabrication. Hence welding adds a step, not just a filler.
Where 400 Wins
400 costs less and forms more easily. It also holds a wider corrosion record in hydrofluoric acid. A tank, a line, or a tube sheet therefore stays on 400. Nickel 201 plate and sheet also competes in hot caustic, where copper contamination matters. Hence the low-load duties stay cheap.
Where K500 Wins
K500 suits a pump shaft, an impeller, a valve stem, or a bolted joint under seawater. Fast flow erodes 400, while the harder K500 surface holds longer. Monel K-500 bar and forging stock covers that duty in the aged condition. Hence high-load marine parts pick K500.
The Temperature Line
400 works to about 480 °C in air, while K500 keeps its aged strength to roughly 400 °C. Above that, K500 overages and loses the gain, so it behaves like 400. Therefore, a hot duty gains nothing from the aged grade.

The Machining Line
Both grades work-harden, so a heavy cut needs a light feed. K500 cuts harder in the aged state, which raises tool wear. A high-volume turned part may prefer a free-machining grade, and Monel R-405 free-machining bar covers that case. Hence machining cost can erase the strength saving.
Corrosion Nuance
K500 gives up a little resistance in some acids, since the precipitate and the aluminium shift the surface behaviour. Seawater and caustic stay close to 400. A severe acid duty therefore stays on 400. Hence the aged grade is a strength tool, not a corrosion upgrade.
The Certificate Difference
400 certifies to B164 as UNS N04400, and K500 certifies under N05500 with the aged condition stated. That condition line matters more on K500, since an annealed bar would fail a strength check. A buyer should read it before machining. Therefore, the certificate type follows the grade.
Where Buyers Get It Wrong
A buyer machines a K500 shaft to final size, then ages it, and the shaft grows out of tolerance. Another welds K500 without a post-weld age, so the seam runs soft. A third buys K500 for a hot 500 °C duty, where the ageing fades. Those three errors cover most of our returns.
What We Do Not Do
We do not melt or roll either grade. We do not age a finished part. Nor do we sell an annealed K500 bar as an aged one, since the certificate would contradict the label.
Those limits keep the grades honest.
Specify Your Order
First, name the grade and the UNS number. Second, state the condition, whether annealed or aged. Then give the form and the size, so the mill order matches the heat treatment.
Related Reading
The grade naming note shows how a designation is built, so a certificate can be read against a trade name.
Frequently Asked Questions
Is K500 stronger than 400? It is, since ageing lifts the yield to about 690 MPa.
Does K500 resist corrosion as well? Close to 400 in seawater, yet slightly weaker in severe acid.
When should a K500 part be aged? After forming and welding, then finished to size.
Which grade suits a pump shaft? K500, because the harder surface resists erosion.
Can 400 be aged? No, since it carries no aluminium or titanium.
- Email: vera.liang@ztwysteel.com
- Location: Xishan District, Wuxi, Jiangsu, China
- Supply range: K500 bar stock, 400 plate on request, R-405 bar, Nickel 201 plate 1–50 mm
- Cutting: length under 4 m, ±1 mm, squareness 1 mm per metre
- Documentation: MTC EN 10204 3.1 with UNS N04400 or N05500, 3.2 on request