What is the difference between Inconel 601 and Inconel 600?

One composition swap separates them. Inconel 600 keeps about 72% nickel, and 601 trades that nickel for chromium and aluminium. 601 lands near 23% chromium with 1.0 to 1.7% aluminium, while 600 sits near 15% chromium with no deliberate aluminium. Jiangsu Zhongtong Weiye Special Steel Co., Ltd. supplies 601 plate, and it books 600 on request.

The Short Answer

601 oxidises better, because its aluminium builds a denser scale. 600 resists caustic and high-nickel duty better, because its nickel share runs higher. Hence the swap buys oxidation and costs nickel, and the price follows that trade.

The Swap in Numbers

600 carries nickel at 72% or more, chromium at 14 to 17%, and iron at 6 to 10%. 601 carries nickel at 58 to 63%, chromium at 21 to 25%, and aluminium at 1.0 to 1.7%. Therefore, 601 moves roughly 12 points of nickel into 6 points of chromium and 1.5 points of aluminium. That single move explains every difference below.

Consequence One — Oxidation Ceiling

600 holds about 1,100 °C in clean air, while 601 holds about 1,200 °C. The aluminium in 601 forms an alumina-rich layer, and that layer diffuses slower than a chromia scale. Hence the extra 100 °C comes from aluminium, not from chromium alone. A furnace above 1,100 °C therefore needs 601.

Consequence Two — Cyclic Duty

A scale that spalls leaves bare metal, and bare metal oxidises fast on the next heat. 600 spalls sooner under cycling, since its chromia scale grows thicker. 601 reheals faster, because alumina forms at low oxygen pressure. Therefore, a batch furnace that cools nightly favours 601.

Consequence Three — The High-Nickel Duties

Nickel resists caustic attack, and it also resists chloride stress cracking in water. 600 carries more nickel, so it holds up in caustic evaporators and in nuclear steam generators. 601 carries less nickel, so it loses some of that margin. Hence a caustic duty picks 600, even though 601 oxidises better.

Consequence Four — Price

Nickel costs more than chromium and iron, so a lower nickel share usually lowers the price. 601 often quotes below 600 per tonne, and the gap tracks the nickel market. Therefore, a hot furnace part often costs less in 601 while performing better.

Where They Agree

Both grades report at least 550 MPa tensile, 240 MPa yield, and 30% elongation in the annealed state. Both weld with ERNiCr-3 filler, and neither needs preheat. Neither carries molybdenum, so neither handles hydrochloric acid. Hence the two are interchangeable in a mild furnace, and the price decides there.

The Carburising Case

A carburising atmosphere attacks the scale, and 601 resists that attack better, since alumina tolerates carbon. 600 also survives, yet its scale degrades faster above 1,000 °C. Therefore, a carburising retort usually takes 601.

The Nuclear Case

A nuclear steam generator tube takes 600, since that duty needs high-nickel corrosion behaviour in pure water. 601 does not carry the same service history there, so a specification rarely allows it. Hence the choice follows the code, not the data sheet.

The Caustic Case

A caustic concentrator takes 600, because nickel resists hot hydroxide. 601 sees attack at the liquid line, since its lower nickel share offers less margin. Therefore, an alkali duty stays on 600 or moves to Nickel 201, not to 601.

Inconel 601 and Inconel 600 plate samples compared after 1,150 °C air exposure

The Sulphur Case

Both grades fail in a sulphur-rich furnace, since nickel sulphides break the scale. 601 fails above roughly 800 °C, and 600 fails at a similar level. Hence a sulphur-bearing kiln needs a different family, not a swap between these two.

Which One for a New Furnace

Start with the peak temperature, then the cycle, then the atmosphere. Above 1,100 °C or a daily cycle, choose 601. Below 1,000 °C with caustic or pure water, choose 600. If both fit, compare the delivered price, since the duty does not differ.

Where Buyers Get It Wrong

A buyer specifies 600 for a 1,150 °C retort and finds scale spalling in months. Another specifies 601 for a caustic evaporator and finds thinning at the liquid line. A third treats the two as identical and changes grade mid-project, which forces a re-qualification. Those three errors cover most of our returns.

What We Do Not Do

We do not melt or roll either grade. We do not weld, and we do not anneal a finished part. Nor do we treat 601 as a drop-in for 600 in caustic service, since that swap voids the margin.

Those limits keep the advice honest.

Specify Your Order

First, name the grade and the UNS number. Second, give thickness, width, and length. Then state the peak temperature and the atmosphere, so we can confirm the ceiling.

Inconel 601 plate and sheet covers retorts and trays. For a 1,000 °C strength part, Inconel 617 coil and strip fits better. For hot corrosion duty, Inconel 625 plate and sheet fits better.

Related Reading

Grade naming systems read best in the silicon steel grade note, since both explain how a spec is encoded. Cut-length practice appears in the cut-to-size note.

Frequently Asked Questions

Is 601 stronger than 600? No, since both report about 550 MPa tensile in the annealed state.

Which grade handles caustic? 600, because its nickel share runs higher.

Which grade handles 1,200 °C? 601, since alumina holds its scale at that heat.

Can 601 replace 600 in a nuclear plant? Rarely, since the specification follows a service history.

Do either handle hydrochloric acid? No, because neither carries molybdenum.

  • Email: vera.liang@ztwysteel.com
  • Location: Xishan District, Wuxi, Jiangsu, China
  • Supply range: 601 plate 1–50 mm, 617 coil 0.5–3 mm, 625 plate 1–50 mm
  • Cutting: length under 4 m, ±1 mm, squareness 1 mm per metre
  • Documentation: MTC EN 10204 3.1 with UNS N06601, 3.2 on request