What is stacking factor of silicon steel laminations?

The stacking factor of silicon steel laminations is the net steel thickness divided by the measured stack height, and it typically lands between 0.93 and 0.97. Consequently, a core quoted at 0.96 already loses 4% of its apparent volume to coating and air. Jiangsu Zhongtong Weiye Special Steel Co., Ltd. supplies coil whose coating build sets that starting number. Below, therefore, is where the ratio leaks and what it costs.

The Definition in One Line

Multiply nominal gauge by sheet count, then divide by the measured stack height. A result of 0.95 means 95% of the stack carries flux, while 5% carries nothing. Hence the core’s effective area is smaller than its drawing suggests.

Four Places the Ratio Leaks

Leak 1 — coating build. Insulation film adds 1–3 µm per side, so a 0.27 mm sheet loses proportionally more than a 0.50 mm one. Therefore, thin gauge always starts lower.

Leak 2 — slitting and edge burr. Burr holds layers apart at the edges, since contact sits on the raised rim. Consequently, burr below 0.02 mm protects the ratio.

Leak 3 — punching bulge. Stamping rolls the edge and bows the centre, which adds a few percent of gap. Hence die clearance and sharpness matter as much as steel grade.

Leak 4 — clamping and step-lap. Interleaved or step-lap joints reduce contact area slightly, and low clamping pressure leaves air pockets. In practice, pressing to a defined load recovers most of that loss.

Typical Bands by Gauge

  • 0.50 mm non-oriented: 0.96–0.97.
  • 0.35 mm non-oriented: 0.95–0.96.
  • 0.27 mm oriented: 0.94–0.96.
  • 0.23 mm oriented: 0.93–0.95.
  • 0.20 mm specialty: around 0.93.

Each step down in gauge spends part of the ratio, so thin gauge trades build height for loss.

The 0.96 to 0.94 Example, Costed

Take a 1000 kVA transformer designed at 0.96. If the delivered stack measures 0.94, effective area falls about 2.1%, so flux density rises 2.1% at constant voltage. Core loss therefore climbs roughly 4%, because loss follows induction near the 1.8 power.

For a unit energised continuously, that 4% becomes a permanent bill. Moreover, winding temperature rises, and insulation life shortens accordingly.

Measuring Without Fooling Yourself

Measure with a micrometer and a flat anvil, and clamp to a stated load, commonly in the 0.1–0.5 MPa range. Record sheet count, then compare against mill gauge on the same basis, before or after coating.

Sampling matters too, since a 20-sheet sample hides lot variation. Therefore, measure at three stack positions, and repeat on every incoming lot.

What to Put in the Purchase Order

  1. Nominal gauge, with a coating basis.
  2. Coating type and target film weight.
  3. Burr limit, typically under 0.02 mm.
  4. Minimum stacking factor at defined clamping pressure.
  5. Gauge tolerance, since ±0.02 mm shifts the ratio directly.

Vague wording invites substitution, and substitution shows up as heat rather than as paperwork.

Why It Bites Motors Differently

In motors, a lower ratio shrinks effective slot area and distorts the air gap, since stack length no longer matches the drawing. Consequently, torque falls slightly and no-load current rises. Moreover, the extra current raises copper loss, which compounds the iron loss penalty.

Hence motor designers often accept 0.95 rather than chase 0.97, because slot fill and manufacturability dominate there.

Standards and Data Sources

IEC 60404-2 governs loss measurement, and gauge certificates usually state the coating basis. Our flux density note explains how B responds to reduced area, while the transformer efficiency explainer ties it to no-load loss.

Lamination stack measured with a micrometer to determine stacking factor

Frequently Asked Questions

 

Can stacking factor reach 1.0?

Never, since coating and contact gaps always occupy space.

Which gauge gives the highest ratio?

Usually 0.50 mm, because coating shares a smaller fraction.

Does clamping pressure change the ratio?

Yes, and low pressure leaves air gaps that no certificate reflects.

Is a lower ratio always worse?

For transformers yes, while motors often tolerate it for other gains.

How is the ratio verified?

By measuring a known sheet count under a defined load.

What We Do Not Do

  • We do not roll, anneal, or coat steel.
  • We do not stamp laminations.
  • We do not measure finished stacks.

Consequently, we state gauge and coating basis, and your QA owns the final number.

Specify Your Order

  1. State grade and gauge with its basis.
  2. Give coating type and burr limit.
  3. Give slit width and tonnage, then confirm port.

M5 Grain Oriented Electrical Steel ships at 0.27–0.30 mm for transformer cores, while M36 Non Oriented Electrical Steel covers 0.50 mm motor duty. Quotes return within one working day.

  • Email: vera.liang@ztwysteel.com
  • Location: Xishan District, Wuxi, Jiangsu, China
  • Supply range: CRNGO M19–M47 at 0.35–0.65 mm, CRGO M4/M5 at 0.23–0.35 mm
  • Slitting: 20–1250 mm, ±0.05 mm, burr under 0.02 mm
  • Documentation: MTC EN 10204 3.1, gauge and coating basis stated, core loss per ASTM A343 / IEC 60404-2