What is the core loss of 27QG120 silicon steel?
The core loss of 27QG120 is 1.20 W/kg as a maximum, measured at 1.7 T and 50 Hz. That figure defines the grade, and every other property follows from it. The sheet itself is 0.27 mm high-induction grain-oriented strip. Jiangsu Zhongtong Weiye Special Steel Co., Ltd. supplies it against that figure.
The Answer in One Number
One number answers the question, namely 1.20 W/kg at 1.7 T and 50 Hz. Everything else in the code, including gauge and grade family, supports that value. Therefore, quote the number first, and quote the qualifiers immediately after.
Qualifier 1 — The Induction Basis
Loss depends on flux density, so 1.7 T must travel with the figure. At 1.5 T the same sheet loses roughly 30% less, which flatters any comparison. Consequently, a 1.5 T figure and a 1.7 T figure cannot sit in one column.
Qualifier 2 — The Frequency
Frequency scales loss, and 50 Hz is the base here. At 60 Hz the figure rises to roughly 1.5 W/kg, since eddy and hysteresis terms both climb. Therefore, a North American project needs a converted number, not a copied one.
Qualifier 3 — The Word Maximum
The 1.20 figure is a guaranteed ceiling, not a typical reading. Mills usually deliver slightly below it, because the test lot must pass the limit. However, design calculations should use the ceiling, since that is what the certificate promises.
Why the Certificate Value Differs From the Design Value
Designers work with worst case, since insulation ageing follows temperature. Mills test one coil per batch, so the certificate reflects a sample. Consequently, a small gap between the two figures is normal. Therefore, never treat a best-case reading as the design basis.
Qualifier 4 — The Gauge
The leading 27 means 0.27 mm, which sets eddy loss and stacking behaviour. Thinner sheet would lower loss, although it raises price and handling risk. Thicker sheet would cost less, yet the loss limit would fail.
Hence the gauge and the number are one decision.
What the Letters Mean
The letter Q marks a grain-oriented grade, and G marks high induction. A plain Q grade guarantees B800 of about 1.80 T, whereas QG requires about 1.88 T. Consequently, the G raises magnetisation performance without changing the loss limit.
Two letters, one added benefit.
What Else the Certificate Lists
The sheet also gives B800, which pairs with the loss figure. Stacking factor appears beside it, because coating weight reduces the steel share. Hence read the certificate as a set of three numbers. Both values matter when you size a core.
What the Loss Does in a Real Core
Take a 1000 kVA unit with a 1.2 t core, which is a common build. At 1.20 W/kg the core dissipates about 1.44 kW at rated flux. That matches the 1.2–1.5 kW no-load band quoted for such transformers.
The arithmetic is short, and the answer is checkable.
What That Costs Over Time
Capitalised at roughly €14 per watt, 1440 W carries a lifetime value near €20,000. Therefore, a 0.10 W/kg difference between two offers is worth about €1,700. That is why buyers negotiate the last decimal.
At 60 Hz and Other Bases
Convert the figure before comparing, since bases differ across markets. A 60 Hz value near 1.5 W/kg is normal for this gauge. Then convert to your own flux density, because cores rarely run at exactly 1.7 T.
When This Grade Is the Wrong Choice
Large power transformers usually want 0.23 mm sheet, since no-load loss dominates there. Small distribution units often accept 30Q or 35Q grades, because price matters more. Therefore, 27QG120 suits the middle band, not every duty.
Neighbouring Grades in the Same Gauge
27QG110 sits one step lower in loss, and 27QG130 one step higher. A step of 10 costs roughly a few percent per ton, and saves proportionally less energy. Hence the middle grade often wins on payback.
What Changes If You Need 0.23 mm Instead
A 23Q090 sheet loses about 10% less, since it is thinner and often domain-refined. Yet it costs noticeably more per ton, and it punches with more care. Therefore, that upgrade belongs in large units, where the loss runs every hour.
Related Reading
Gauge tiers and stock coverage appear in the oriented grades note. Directional behaviour is explained in the oriented versus non-oriented note.

Frequently Asked Questions
A maximum, since the certificate guarantees a ceiling.
1.7 T, because transformer cores work near that level.
High induction, which lifts B800 to about 1.88 T.
Yes, although the loss rises to roughly 1.5 W/kg.
No, since price and stacking both worsen.
A Sanity Check on Delivery
Compare the certificate to the purchase order first, since typos happen. Then check gauge with a micrometer, because tolerance drifts within the band. Finally, verify coating class, since oil and air demand different surfaces. Even then, keep one sample per lot, so disputes have evidence.
What We Do Not Do
We do not test loss in-house on a single-sheet rig. We do not quote a figure without a basis. Nor do we sell 27QG120 against a 1.5 T table.
Those limits keep the number comparable.
Specify Your Order
First, state the required W/kg and its basis. Second, give the slit width. Then confirm the coating class, so we can match stock or programme.
M5 Grain Oriented Electrical Steel covers this 0.27 mm band, and M4 Grain Oriented Electrical Steel covers thicker builds. Quotes return within one working day.
- Email: vera.liang@ztwysteel.com
- Location: Xishan District, Wuxi, Jiangsu, China
- Supply range: CRGO 0.23–0.35 mm, 23Q085 to 35Q150, coating C5 or C6
- Slitting: 20–1250 mm, ±0.05 mm, burr under 0.02 mm
- Documentation: MTC EN 10204 3.1, loss data per ASTM A343 / IEC 60404-2