How does silicon content affect the magnetic performance of non-oriented electrical steel?

Silicon moves four properties at once, and only one of them helps. Adding a percent raises resistivity by roughly 12 micro-ohm-centimetres and lowers saturation by about 0.04 T. Silicon content therefore trades loss against punchability, not loss against nothing. Jiangsu Zhongtong Weiye Special Steel Co., Ltd. supplies grades from 1.5% to 3.5% silicon.

The Baseline at 1% Silicon

A 1% grade is rare in production, yet it sets the reference point. Low-silicon sheet conducts flux well and punches easily, although it saturates late. Its resistivity sits near 23 micro-ohm-centimetres, so eddy currents flow freely. Hence loss stays high, which suits cheap, slow machines.

Step 1 — From 1% to 2%

Resistivity climbs to roughly 36, so the eddy term falls to about 64% of its earlier value. Saturation drops by 0.04 T, and hardness begins to rise. That single step buys most of the available gain.

One percent, one third of the eddy loss.

Step 2 — From 2% to 3%

Resistivity reaches about 48, and eddy loss falls again, although the slope flattens. Hardness now bites, since dies wear faster and edges burr sooner. Therefore, punch shops often stop at 2.5% or 3.0%.

Step 3 — From 3% to 3.5%

The last half percent buys about 4% more resistivity, so the price looks steep. Saturation falls to roughly 1.98 T, which narrows the design window. Cracking risk also rises during cold rolling and slitting.

Hence 3.5% marks the practical ceiling.

Why Mills Add Silicon at All

Mills add silicon to cut eddy loss, since it is the cheapest lever available. Alloying costs less than an extra rolling pass or a thinner gauge. Hence silicon remains the first tool in grade design.

The Two Mechanisms

Resistivity governs eddy loss, since current meets more resistance in a doped lattice. Anisotropy governs hysteresis, and silicon lowers it slightly by softening the crystal directionality. Both effects push loss down, although resistivity does most of the work.

The Gauge Interaction

At 0.50 mm, resistivity dominates the loss, so silicon pays well. At 0.35 mm, eddy loss is already small, so silicon adds less. Therefore, the same silicon step matters more on thick sheet.

Where Saturation Bites

Tooth flux in a compact motor can reach 1.7 T, and peak flux during inrush goes higher. A 3.5% grade with 1.98 T saturation leaves a thinner margin than a 1.5% grade. Consequently, high-silicon sheet suits stators with generous iron, not cramped ones. That is why traction motors often stay near 3.0%.

The Hysteresis Side of the Ledger

Hysteresis falls modestly with silicon, since domain walls move more freely in a cleaner matrix. The gain rarely exceeds a few percent per point of silicon. Therefore, hysteresis alone cannot justify a premium grade.

Punchability and Die Life

Hardness rises with silicon. A 3% sheet wears a die roughly twice as fast as a 1.5% sheet. Sharp edges and tight clearances make that gap worse. Hence tooling budget enters the grade decision.

What a Half-Point Step Is Worth

Moving from 2.5% to 3.0% typically cuts loss by 3% to 6%. That is a small number against a die-life penalty of 10% or more. Consequently, the step is often skipped in high-volume press shops.

Where Buyers Get Surprised

A buyer replacing 50W600 with a higher-silicon 50W470 finds burr growing, since the edge work-hardens sooner. Burr bridges laminations, so real loss lands above the catalogue value. Hence the grade change needs a trial coil, not a spreadsheet.

What Silicon Does to Welding

Higher silicon promotes brittle phases at the weld, so joints crack more easily. Builders often weld the frame and clamp the core instead. Consequently, a high-silicon grade pushes the assembly method toward mechanical clamping.

Aging and Carbon

Silicon does not remove carbon, so mills decarburise separately. Residual carbon lets loss creep upward over years, which is why annealing matters. Therefore, chemistry and anneal belong in one conversation. A poor anneal undoes much of the alloy gain.

Silicon and Heat Treatment

Annealing does not change silicon, yet it changes how silicon behaves. A clean matrix lets the resistivity benefit show fully. Therefore, loss figures assume a proper final anneal.

How to Read Silicon on a Certificate

Certificates state silicon as a range, since mills control a window rather than a point. Loss is measured on the finished coil, so the range explains batch scatter. Hence ask for both, and compare them together.

Two numbers, one grade.

What Changes in Your Design

Because loss per kilogram falls, a higher silicon grade shrinks the core slightly. It also narrows the flux margin, so the tooth width may grow instead. Therefore, a grade change usually forces a redesign, not just a substitution.

Related Reading

Grade families appear in the NGO grades note, and the loss basis appears in the M15 note.

Silicon content range printed on a non-oriented electrical steel coil certificate

Frequently Asked Questions

Does more silicon always mean lower loss?

Usually yes, although the gain flattens near 3.5%.

Does silicon raise or lower saturation?

It lowers saturation by about 0.04 T per percent.

Why do punch shops resist high silicon?

Dies wear faster and edges burr sooner.

Is 1.5% silicon still useful?

Yes, for cheap slow machines with generous iron.

Does silicon affect corrosion?

It helps slightly, and coatings do more.

What We Do Not Do

We do not roll steel, since mills own that step. We do not promise a silicon figure below the certificate range. Nor do we sell a grade as punchable when it is not.

Those limits keep the trade-offs visible.

Specify Your Order

First, state the loss class you need. Second, give gauge, width, and tonnage. Then mention your die condition, so we can warn you before a grade bites.

M36 Non-Oriented Electrical Steel covers standard motor duty. M19 Non-Oriented Electrical Steel suits the M19 class. Reactor Core Lamination serves gapped cores.

  • Email: vera.liang@ztwysteel.com
  • Location: Xishan District, Wuxi, Jiangsu, China
  • Supply range: CRNGO 0.35–1.00 mm, silicon 1.5% to 3.5%
  • Slitting: 20–1250 mm, ±0.05 mm, burr under 0.02 mm